Tg of bands or PLC bands. So, the work hardening capacity of AIMg6.5 alloy is reduced due to the 
ta Ptüperties inhomogeneous deformation at room temperature (£pom<M). 
v au ling Fig.2 illustrates the position of fracture surfaces in respect to the tensile axis for thinner sample with 
“a Tab high w/f ratio (w/t=8.3) and for thicker sample with low w/f ratio (w/t=2.8). 
ned, py 
“18 reduction 
) Rerystallizeg 
lat is Cased by 
Ste Hall-Pegh 
63 | fl 
1809 18: 
HY 
Fig.2: The position of fracture surfaces on the tension specimen with: a, b) fine-grained fully 
recrystallized structure (w/t=8.3); c, d) coarse-grained non-fully recrystallized structure (w/r=2.8). 
AIMg6.5 alloy 
3m temperature 
racterized by On the thinner specimens with fine-grained fully recrystallized structure and high w/t ratio, 
is induced by w/t=6.3+8.3 (Fig.2a), the failure occurs along the plane which is inclined at ~60-70° to the tensile 
a It was also direction. The fracture surface was almost parallel to the PLC bands, which are clearly visible on 
he tested allo that specimen surface, and oriented at £60° to the tensile axis (on the broad specimen face, Fig.2b). 
vas eminated As the plastic strain ratio in the tested material was about R~0.55 in the rolling direction [10], the 
st beyond the angle of localized necking, according to the Hill’s theory [12], should be about 6~59°. It means that 
wtead in other the PLC bands make a regions of localized necks, and later at these places the fracture appearance is 
content [6-9 favorized. In the case of thicker sample with coarse-grained non-fully recrystallized structure and 
ıtween uniform low w/t ratio, w/f=2.5+5 (Fig.2c,d), PLC bands are less evident and the failure occurs at ~55° 
ei) and work through the specimen thickness (Fig.2c) at an orientation of 90° to the tensile axis on the broad 
tested M63 specimen face (Fig.2d). However, having in mind that the appearance of PLC bands was suppressed 
e uniform sin in coarse-grained samples (Fig.2d), it was assumed that there were no places of strain localization, 
dos] parallel to PLC bands, but the fracture surface corresponds to localized shear banding in the planes 
a te pod with maximum shear stress through thickness. A fractographic study of AIMg6.5 tensile specimens 
m due fo neck using scanning electron microscope (SEM) has shown transgranular ductile dimple fracture (Fig.3). 
fond 85 18 
maximum load. 
iy parameters 
try (Fig.]) The 
zo found rather 
value of 031 
structure it Was 
ed that negative 
also causes the 
ag shear failure 
at. within. Shear Fig.3: SEM fractographs of AlMg6.5 tension specimens with a) coarse-grained non fully 
recrystallized structure (w//2.8) and b) fine grained fully recrystallized structure (w//=8.3). 
2367
	        
Waiting...

Note to user

Dear user,

In response to current developments in the web technology used by the Goobi viewer, the software no longer supports your browser.

Please use one of the following browsers to display this page correctly.

Thank you.