Full text: Fortschritte in der Metallographie

Prakt. Met. Sonderband 38 (2006) 301 
ure and 
Cc matrix 1000 
les are 
rdening 800 
LONGITUDINAL 7 
= TRANSVERSE 
e dual- > 600 
spect to z 
X 400 4 
FF 
N 
| LONG. TRANSV. 
200 lo2%ys 612 616 
TE 18.06 1288 
%E, 2547 2738 
0 
national ) 5 10 15 20 25 30 
period. ELONGATION (%) 
; to the Fi . 
ig. 1. Tensile test curves of the as-rolled steel. 
factory 
‘omoter 
charge 1000 - 
ip Eng, 
RALIA- 800 
stly, we Be 
aL Tx TRANSVERSE 
pickling © | LONGITUDINAL 
= 600 
3 
#4004 
FE 
@ 1 
; LONG. TRANSV. ! 
200 | 020vs 725 746 
| TS 798 810 
%Eu 14.58 14.19 
| %E; 27.7 2368 es 
0 _ 
sat. J 5 10 15 20 25 30 
ELONGATION (%) 
-87. : : 
ie Fig. 2. Tensile test curves of the specimens treated at 620°C for 2 h. 
ia, 
1000 - 
Pub. 
800 
de 
600 | 8 
400 
FE 
wn 
‘GC! I ~ "7 LONG. TRANSV 
200 0.2%YS 494 454 
TS 751 760 
[Er ZF ZZ 
ad IL 
0 5 10 15 20 25 30 
ELONGATION (%) 
Fig. 3. Tensile test curves of the specimens normalized at 920°C for ¥; h. 
fy
	        
Waiting...

Note to user

Dear user,

In response to current developments in the web technology used by the Goobi viewer, the software no longer supports your browser.

Please use one of the following browsers to display this page correctly.

Thank you.