Full text: Fortschritte in der Metallographie

310 Prakt. Met. Sonderband 38 (2006) 
Composition: rT 
Fe 0.3550.0.62510.855Mn.0.047Ni,2.35Cr.0.42Mo,0.1 av. [cea =r 
0.006Co,0P,08,0.011N,0.00018,0.07Cu (wt.%) Fa 
‘wustenite Grain Size = 0.00015 m, Cooling Rate = SK/s YHH = 543 
uu oe 
= — Martensite 
sc 7 +... Bainite 
° 
0.001 0.01 0. Cooling Rate, (K/s) 10 100 1000 
Figure 3. Sample “A” [6]. 
=> i ed 
Lmposition: = 
sin ATO TA FR 2v, Ee 
1.005Co,0P,08,0.011N,0.00018,0.021Cu {wt. 5% 
yustenite Grain Size = 0.0001 Sm, Cooling Rate = SK/s Ci YHN = 556 
"700 —— i 
7 x — Martensite 
£ | Bainite 
“ a0 - WERE u Ferrite 
\ 60- 
Sn 
0 A ERE PR pS Y, 
0.001 0.01 a RL 100 1000 
Figure 4. Sample “B” [6]. N: 1 
N+N 
N+V 
HARDNESS AFTER OIL QUENCHING N+p 
500 
475 
~ 450 
fy 
5 425 
x 
wv 400 
~~ 
0 
= 375 
m 
T 350 
325 
300 
Poleshoe ID. 
@ Upper face @ Lower Face 
Fir 
1 
gure 5
	        
Waiting...

Note to user

Dear user,

In response to current developments in the web technology used by the Goobi viewer, the software no longer supports your browser.

Please use one of the following browsers to display this page correctly.

Thank you.