Full text: Fortschritte in der Metallographie

Prakt. Met. Sonderband 38 (2006) 311 
HARDNESS AFTER TEMPERING 
400 
390 
380 
32 370 m 
> 360 368 
© 350 
= 340 
© 330 
320 
310 
300 
Poleshoe 
0 Upper face @ Lower Face 
Figure 6 
Table IV. Hardness of poleshoes “A” and “B” after each thermal treatment 
SAMPLE HB 
A (N) 311 
A (N +N) 390 
A (N +N +WQ) | 455 
A(N+N+WQ+R 264 
ß (BM) 301 
B (BM + N) 371 
B (BM + N+ N) 381 
B(BM+N+N+WQ) 525 
IB(BM+N+N+WwQ+R 264 
N: 1° Normalizing 
N+N: 2"! Normalizing 
N+WQ: Double Normalizing, followed by water Quenching. 
N+N+WQ+T: Double Normalizing, followed by water Quenching and Tempering 
Table V. 
CHARPY TEST ISO KCV (20 °C) 
Poleshoe Mean (J) 
- | 13.02 | 7 - 
v 12.62 12.5 
11.83 
-. 7 
„ 18.94 Teo 
18.28 
TT 4381 
‚u 38.09 36.4 
23 44 
{ 
E 
9 ‘QF 
fr >
	        
Waiting...

Note to user

Dear user,

In response to current developments in the web technology used by the Goobi viewer, the software no longer supports your browser.

Please use one of the following browsers to display this page correctly.

Thank you.