348 Prakt. Met. Sonderband 38 (2006)
2. EXPERIMENTAL PROCEDURE Th
Aft
The leaky heat exchanger (Fig. 1) was cut in several directions with a hacksaw. By optical To
inspection only minimal corrosion in the region of the water side is observed (Fig. 2). The etc
oil side shows a copper coloured surface and at the water side the surface is brown with -
minimal green corrosion dots. Using a sectioning machine samples were taken from
several regions for metallographic preparation (Fig. 3).
Fol
The
ele
3.
3.1
The
Fig. 1: Plate heat exchanger she
Th
(h} oil oir water vr The
inv
gre
oil out
water in
1:
Fig. 2: Part from the plate heat exchanger (oil and water side; Fic
Green corroded dots are visible in (a)
3.2
At
the
cof
gre
bot
the
an
wit
Fig. 3: Plate heat exchanger and marks for the sampling at the water side a
or