Fig.7: X-ray diffraction patterns recorded with Cu radiation for the Al-4wt% Ni.
a. as cast, b. as melt-spun fibers. (A Al3Ni; m Al
The high Ni alloys have been rapidly solidified by the melt extraction method. When
normally cast in conditions of slow cooling the Al-Ni alloys having a Ni content of 10.3 up to
28.2wt % Ni consist of primary dendrites of AlNi compound and of the (Al + Al3Ni) eutectic
mixture — fig.8 and fig.10 -. The alloy richer in Ni, namely Al — 31.4wt % Ni has a different
microstructure ~ fig 12 -. Actually its solidification started by separating the Al;Niz primary
RS crystals, that later were involved in a peritectic reaction giving rise to the compound Al3Ni
(composition
"8 Core
uted by apphing ;
2 “rm wide, 0.02-
asing the cooling
tie changes in the
the obtention Of 2
15 also ascertained
Ni richest alloy 18
an intensity ps
IN ¢ oe
uo eed) Fig.8: Slowly solidified Al-24.2 Fig.9: Rapidly solidified Al-24.2
wt% Ni. SEM electron micrograph wt% Ni. SEM electron micrograph
(composition image x150). (composition image x600).